How do you repair-weld cast iron?
A successful repair weld in cast iron largely comes down to minimising three things during welding.
1. Residual welding stresses
Cast iron is relatively brittle and struggles to absorb the thermal stresses created by welding. The material in and around the joint must be able to cope with those stresses to avoid cracking.
Tip: Lightly peen the bead straight after welding and choose a nickel-based filler metal that is insensitive to carbon pick-up from the base material. That gives a tough weld metal with a low yield strength that absorbs as much of the stress as possible.
2. Heat input
Rapid heating and cooling make the heat-affected zone hard, brittle and crack-prone – which also makes machining after welding harder. Hardness depends on the cooling rate, and the width of the zone on the heat input.
Tip: Plan the bead sequence, weld short beads without weaving and use a low current. Vertical-down welding has proven to give low heat input.
3. Stress concentrations
In parts with complex shapes – tight angles and transitions between thin and thick sections – areas some distance from the weld may need preheating so that they go through a similar thermal cycle as the joint. This is sometimes called indirect preheating.
Hot or cold welding?
- Hot welding: The whole workpiece is heated to about 600 °C before welding and then cooled slowly, for example in a furnace. Used for complex parts where neither expansion nor shrinkage can occur freely. The filler metal matches the base material.
- Cold welding: Nickel-based electrodes (over 50 % nickel) dissolve high carbon contents without the weld metal becoming hard. Weld with the lowest possible current, short beads (no longer than twice the electrode diameter) and peen after each bead. Usually the fastest and cheapest method.